To be applied on surfaces primed with the primer « EPO SS » or on mortars obtained with « EPO SS».
Preparation of the product
.Mix the product according to the following ratio by weight: Component A: 100 Component B : 25 Mix Component A separately and then add Component B
Self – leveling preparation
Add to the mixture (A + B) 70 parts of spheroidal quartz inert material (0,1 - 0,5) with a low speed mechanical mixer.
Pot life
40 minutes at 20° C
Environmental conditions
Ambient temperature: from + 10 to 35° C Temperature of the support: > 10° C Humidity: 0 - 85 % In order to prevent the formation of condensation, it is necessary that the temperature of the substrate is at least 3° C above the dew point.
Drying and hardening time
For the thickness of 300 microns 10° C 20° C 30° C Dry to touch 8 3 1 hours Dry in depth 16 8 5 hours
Time of overpainting
Minimum (hours) 10° C 20° C 30° C 10 8 5 hours Maximum (days) 7
Application
As a finish: roller, for small touches, use the brush. As a self - leveling product: serrated spatula and bubble breaking roller. If you use the roller, you have to use medium - haired rollers.